According to the characteristics of a low-grade zinc-pyrite-Iron ore,several processing solutions were compared,then detailed reagent condition tests and close-circuit tests were carried on.The results showed that:with adopted pyrite selective flotation-zinc flotation-magnetic separation flowsheet,Zn /S /Fe separation was effectively actualized.A pyrite concentrate with a S grade of 46.51% and a recovery of 93.70% was obtained.Meanwhile,a zinc concentrate with Zn grade and recovery of 47.16% and 55.23%,a iron ore concentrate with Fe grade and recovery of 66.54% and 28.18%,respectively,can be reclaimed.%根据某低品位锌硫铁多金属矿矿石的原矿性质,进行了多种流程方案的对比、详细的药剂条件试验和闭路试验研究。试验研究结果表明:采用硫优先浮选—锌浮选—磁选工艺流程,成功实现了锌硫铁的分选,获得硫精矿含 S 46.51%,回收率为93.70%;锌精矿含 Zn 47.16%,回收率为55.23%;铁精矿含铁66.54%,回收率为28.18%的理想指标。