FIELD: metal working. SUBSTANCE: steel parts are put into iron box with solid carburizer and heated to 930 C. Cementation is conducted to 1 mm depth. Parts are cooled in boxes under air atmosphere to 680-550 C, kept for 0.3-0.5 h at this temperature, heated to 800-820 C, and quenched. EFFECT: increased durability of parts, speeded up production, and improved operational conditions. 2 cl, 1 tbl
机译:领域:金属加工。实质:将钢制零件放入装有固体渗碳剂的铁箱中,并加热至930℃。固结至1毫米深。将零件在空气气氛下的盒子中冷却至680-550 C,在此温度下保持0.3-0.5 h,加热至800-820 C,然后淬火。效果:提高了零件的耐用性,加快了生产速度并改善了操作条件。 2厘升,1汤匙