Antimony in antimony-bearing gold concentrates was recovered by alkaline sodium sulphide leaching,and segregation-free electrodeposition.Based on small-scale experiment,industrial practice was carried out according to actual conditions of production site.After optimization of process parameters of electrodeposition,comprehensive leaching rate of antimony is 96.72%,purity of cathode antimony is 96.36%,antimony concentration in barren liquor is 5.54 g/L,comprehensive current efficiency is 63.84%,and NaOH consumption for one ton antimony is 617.2 kg.%采用碱性硫化钠浸出—无隔膜电积的方法回收含锑金精矿中的锑,在小型试验基础上根据生产场地的实际情况进行了工业实践.通过对电积过程工艺参数优化,锑综合浸出率为96.72%,回收阴极锑纯度96.36%,贫液含锑5.54 g/L,综合电流效率63.84%,吨锑氢氧化钠消耗量617.2 kg.